< Zurück
rfa-ringversuch
2003 - RFA Ringversuch GeoPT13 - Loess
Veranstalter des Ringversuchs
nternational Association of Geoanalysts and Geostandards Newsletter - GeoPT13
Ringversuchsmaterial
Loess
Literatur
Proficiency Testing Report GeoPT13 (Laborcode CRB = N3)
Hauptelemente [MA%]
CRB
RV
1sRV
Z-Score
Na₂O
1,160
1,058
0,021
---
MgO
2,950
2,900
0,049
---
Al₂O₃
6,120
6,200
0,094
---
SiO₂
53,410
53,240
0,560
---
P₂O5
0,145
0,130
0,004
---
K₂O
1,360
1,300
0,025
---
CaO
16,650
16,310
0,210
---
TiO₂
0,437
0,423
0,010
---
Fe₂O₃ tot
2,130
2,100
0,038
---
MnO
0,070
0,064
0,002
---
Spurenelemente [µg/g]
CRB
RV
1sRV
Z-Score
Ba
230,00
201,00
7,21
---
Ce
47,00
53,00
2,32
---
Co
10,00
5,95
0,36
---
Cr
112,00
105,70
4,20
---
Cu
12,00
11,31
0,63
---
Ga
5,80
7,08
0,42
---
Hf
8,00
9,10
0,52
---
Nb
7,50
8,60
0,10
---
Ni
23,00
23,30
1,20
---
Pb
12,00
11,30
0,63
---
Rb
53,00
51,20
2,33
---
Sr
304,00
279,00
9,50
---
V
46,00
37,60
2,45
---
Y
47,00
47,10
1,74
---
Zn
36,00
34,40
1,60
---
Legende
CRB
Ringversuch
1s-RV
Z-Score
*
Ergebnisse CRB
Ergebnisse Ringversuch
Standardabweichung Ringversuch
Differenz des Messwerts vom Mittelwert des Ringversuchs
Wert nicht zertifiziert